| 性能 | 
				ASTM A240和 ASME SA-240  要求的低機械性能  | 
		||
| 304 | 304L | 304H | |
| 
				0.2% 抵消 屈服強度, psi MPa  | 
			
				 30,000 205  | 
			
				 25,000 170  | 
			
				 30,000 205  | 
		
| 
				極限抗張強度, psi MPa  | 
			
				 75,000 515  | 
			
				 70,000 485  | 
			
				 75,000 515  | 
		
| 延伸百分比(2英寸或51mm) | 
				 40.0  | 
			
				 40.0  | 
			
				 40.0  | 
		
| 
				硬度, 大., 布氏硬度) RB  | 
			
				 201 92  | 
			
				 201 92  | 
			
				 201 92  | 
		
| 測試溫度 | 
				 0.2% 屈服強度  | 
		||
| °F | °C | psi | (MPa) | 
| -423 | -253 | 100,000 | 690 | 
| -320 | -196 | 70,000 | 485 | 
| -100 | -79 | 50,000 | 354 | 
| 70 | 21 | 35,000 | 240 | 
| 400 | 205 | 23,000 | 160 | 
| 800 | 427 | 19,000 | 130 | 
| 1200 | 650 | 15,500 | 105 | 
| 1500 | 815 | 13,000 | 90 | 
| 抗拉強度 | 延伸 | |
| psi | (MPa) | 百分比 | 
| 250,000 | 1725 | 25 | 
| 230,000 | 1585 | 35 | 
| 150,000 | 1035 | 50 | 
| 90,000 | 620 | 60 | 
| 70,000 | 485 | 50 | 
| 66,000 | 455 | 43 | 
| 48,000 | 330 | 34 | 
| 23,000 | 160 | 46 | 
| 溫度 | 夏氏V形沖擊實驗能量吸收 | ||
| °F | °C | 英尺 ? 磅 | 焦耳 | 
| 75 | 23 | 150 | 200 | 
| -320 | -196 | 85 | 115 | 
| -425 | -254 | 85 | 115 |